Brazing refrigerant pipe: flux, filler rods and map gas
A practical guide to brazing copper refrigerant lines: choosing filler rod and flux, heating with map gas and keeping the joint clean inside.
Related products
- Klima Flux Powder (100 g & 250 g)
- Klima Map Gas (Brazing & Welding)
- Klima Copper Coils & Tubes
- Klima Filter Driers
Why refrigerant joints are brazed
A refrigerant circuit has to hold pressure and vacuum for years. Brazing, which uses a filler metal that melts above 450 °C, gives joints that are strong, vibration-resistant and leak-tight. Soft solder melts at lower temperatures and is not used on refrigerant lines.
Choosing the filler rod
- Copper-phosphorus rods (often 0 to 15 % silver) are self-fluxing on copper-to-copper joints, so they need no flux.
- Silver-bearing rods are used with flux for joining copper to brass or steel, for example at service valves and compressor stubs.
Joint fit and clearance
Brazing filler is drawn into the joint by capillary action, and that works only when the gap between tube and fitting is small and even. For copper-to-copper joints the right gap is roughly 0.05 to 0.2 mm. A loose fit leaves voids that leak under pressure, and a forced fit starves the joint of filler. Use fittings sized for the tube, clean both surfaces and push the tube in to the stop.
When flux is needed
Flux dissolves the oxide that forms as copper heats and protects the joint until the filler flows. Mix Klima Flux Powder with clean water to a paste, brush a thin coat on the outside of the tube and fitting only, and keep flux out of the pipe interior. Flux residue is corrosive, so wash it off with hot water once the joint has cooled.
Heat source: map gas, propane or oxy-acetylene
Map gas burns hotter than ordinary propane, so it heats copper faster and suits the small and medium tube sizes used on split and VRF systems. Oxy-acetylene gives the most heat and is chosen for large pipe sizes and thick sections, but it needs a regulator set and trolley. Whichever you use, follow the flammable-gas safety rules for storage, ventilation and fire watch.
Method in short
- Cut the tube square, ream and clean the end and the fitting with abrasive until bright.
- Assemble with the correct overlap and a small, even clearance.
- Purge the pipe with nitrogen at a low, steady flow so the inside stays free of black oxide scale.
- Heat the tube first and then the fitting, moving the flame evenly around the joint.
- Touch the rod to the joint opposite the flame so the filler is drawn in by the heat of the metal.
- Let the joint cool, wash off any flux, then pressure test with nitrogen and evacuate before you charge.
Why the nitrogen purge matters
Hot copper reacts with oxygen to form a black oxide scale on the inside of the tube. The scale flakes off later, travels with the refrigerant and blocks the filter drier, the metering device or the oil passages in the compressor. A low, steady flow of oxygen-free nitrogen keeps air out of the tube while you braze. Leave a vent open at the far end so that pressure cannot build up inside the pipe and blow through the molten filler.
Reading the heat
Heat the tube and the fitting evenly and let the hot metal, not the flame, melt the rod. At brazing temperature the filler flows into the gap on its own and leaves a bright, continuous line all round the joint. If the rod balls up, the joint is too cold. If the flux turns black or the copper scales heavily, it has been overheated. Stop heating as soon as the filler has flowed all the way round.
Common mistakes
- Heating the rod directly with the flame instead of heating the joint
- Flux inside the pipe, which contaminates the circuit
- Brazing without a nitrogen purge
- Too much filler, which runs into the pipe and can restrict the flow
- Quenching a hot joint with water instead of letting it cool before you wash off the flux
- Brazing while refrigerant is still in the system
Protect valves and driers
Wrap service valves, sight glasses and filter driers with a heat shield or wet cloth, and remove Schrader cores before brazing nearby. Fit the drier last, with the circuit open to nitrogen, so it takes in as little moisture as possible.
Inspect and test the joint
- Look for a smooth, continuous fillet of filler all round the joint with no pinholes or gaps.
- Wash off flux residue with hot water and a brush, then dry the joint.
- Pressure test the circuit with nitrogen to the test pressure given by the equipment maker, and check the joints with soapy water or a leak detector.
- Evacuate to a deep vacuum, with a usual target below about 500 microns, and make sure that it holds before you charge.
Safety on the job
- Keep a fire extinguisher and a fire watch in place, and remove flammable material from the work area.
- Recover the refrigerant before you braze. Heating refrigerant with a flame produces toxic and corrosive gases.
- Use cadmium-free silver-bearing rods.
- Work in a ventilated space, wear eye protection and gloves, and keep gas cylinders upright and secured.
Questions about brazing
Do I need flux for copper-to-copper joints?
Not with copper-phosphorus rods, which flux the joint themselves on clean copper. Use flux with silver-bearing rods and whenever you join copper to brass or steel.
Why is black scale forming inside my pipe?
It is copper oxide, formed when copper is heated with air inside the tube. Purge with nitrogen every time you braze, and flush the line with nitrogen if scale has already formed.
Can map gas braze every pipe size?
It suits the small and medium sizes used on split and VRF systems. Large diameters and thick fittings need more heat, so oxy-acetylene is the better choice there.
Can I use soft solder on refrigerant lines?
No. Soft solder melts below 450 °C and does not give a joint that holds refrigerant pressure through years of vibration and temperature change.